of lpg which may be stored
in such gear. We have no
mind that it will be poor to
prod an exp sum to that area
invest by exp of approx 1 pt petrol.
Some aerofols are press with
lpg gas or propane & altho relat
harm singly should not be stored
in numbers.
The use of layer quant liquifid
gas sh be prohib.
Parafin heaters are also potentive
sources of fire & exp & should
sh be prohib.

Holdsworth Col Appl Science. Univ Leeds
27 Aug 68 A Roberts.

B 406 BRS no date R 3/1/68
All the DPACK failures followed a sim
pattern. Slight spalling of the DP
commenced at about 1/2 max load.
Spalling became prog worse until
at 85-95% of max load a A
wedge of DP fell out all round.
This effectivly reduced bearing
area of DP by 1 1/2" all round.
After failure DP was gen shattered
but in two cases cracks were
discernable in the remaining DP.

Dam to RC block occur in each
test except C2. Dam took form
of cracks emanating from
corners of the T.H. and spalling
of the outer face of 1 or 2
blocks. The TH were severly
distorted in all cases except C2.

DP failed one 29 day DP 21.
load 126 tons.